Research Article

Relationships among the Microstructure, Mechanical Properties, and Fatigue Behavior in Thin Ti6Al4V

Table 2

Summary of the study showing absolute values and variance (%) of properties of AR materials.

Microstructure0.2% proof stressElongationFatigue strength
(MPa)(%)(%)(%)(MPa)(%)

As-received
(equiaxed grain size = 15–20 m)
978013.601800

Bimodal (950A)
(equiaxed grain size = 15–20 m + lamellar width of 2–4 m)
10174.0011.8−13.6158−12.2

Widmanstätten (1050A)
(lamellar width of 10 m + >400 m α grain boundary)
10416.4210.3−24.4153−15

Martensite (1050Q)
(200 m grain size with inside acicular )
111413.87.8−42.7135−25