Optimizing the Parameters of Spark Plasma Sintering to Enhance the Hardness of MgO/TiC Composites

Table 8

Results from experiments sorted by sintering parameters, with emphasis on mean density and signal-to-noise ratio.

Experimental runSintering factor’sResponses (experimental density, S/N ratio)
Sintering temperatureSintering pressureSintering timeTDMean EDSDPorosityMean signal to noise ratio
(°C)(MPa)(minutes)(g/cm3)(g/cm3)(%)(dB)

150035151.811.7210.0357674.574.73617
250045201.811.7410.0021103.574.82660
350055251.811.7610.0258282.1654.95175
455035201.811.7810.0031751.075.04905
555045251.811.7910.0004120.455.10270
655055151.811.8010.0016260.265.11976
760035251.811.7210.0142494.754.71977
860045151.811.7910.0006574.575.07017
960055201.811.8010.0018203.575.11514