Research Article
Investigating the Microstructure, Tensile Strength, and Acidic Corrosion Behaviour of Liquid Metal Stir Casted Aluminium-Silicon Carbide Composite
Table 3
Corrosion experiment values and their corresponding S/N ratios.
| Run | Acidic solution | Immersion time (hours) | Reinforcement (Wt. %) | Corrosion rate (mm/year) | S/N ratio (dB) |
| 1 | HCl | 30 | 0 | 11.66 | −21.33 | 2 | HCl | 56 | 10 | 12.13 | −21.67 | 3 | HCl | 80 | 20 | 14.01 | −22.92 | 4 | HNO3 | 30 | 10 | 9.91 | −19.91 | 5 | HNO3 | 56 | 20 | 11.24 | −21.01 | 6 | HNO3 | 80 | 0 | 7.15 | −17.08 | 7 | H2SO4 | 30 | 20 | 11.46 | −21.18 | 8 | H2SO4 | 56 | 0 | 4.83 | −13.67 | 9 | H2SO4 | 80 | 10 | 12.34 | −21.82 |
|
|