L9 experimental design with results.

Jute fiber percentagePercentage of tile powderChemical treatmentWear index in g/minShore D hardness

53No treatment0.2779
565% NaOH0.1982
5910% NaOH0.1583
1035% NaOH0.2673
10610% NaOH0.2177
109No treatment0.1281
15310% NaOH0.2669
156No treatment0.1972
1595% NaOH0.1177